Grado |
Composición % |
Densidad |
Punto de Cedencia (psi) |
Ultimo Esfuerzo a la Compresión. (psi) |
Dureza Brinell |
Temperatura indicada para el vaciado |
ASTM |
|
Estaño |
Antimonio |
Plomo |
Cobre |
gr/cm3 |
20°C |
100°C |
20°C |
100°C |
20°C |
100°C |
°C |
No.2 |
89 |
7.5 |
0.03 |
3.4 |
7.39 |
6100 |
3000 |
14900 |
8700 |
24.5 |
12 |
424 |
5X |
87 |
9 |
|
4 |
|
6300 |
|
15000 |
|
25 |
13 |
470 |
No.3 |
83.3 |
8.2 |
0.03 |
8.3 |
7.4 |
6600 |
3150 |
17600 |
9900 |
27 |
14.5 |
491 |
|
|
|
|
|
|
|
|
|
|
|
|
|
No.7 |
10 |
15 |
75 |
- |
9.73 |
3550 |
1600 |
15650 |
6150 |
22.5 |
10.5 |
338 |
No.8 |
5 |
15 |
80 |
- |
10.04 |
3400 |
1750 |
15600 |
6150 |
20 |
9.5 |
341 |
Magnolia |
3 |
14 |
83 |
- |
10.6 |
3380 |
1810 |
15500 |
5940 |
18 |
9.3 |
338 |
No.11 |
- |
15 |
85 |
0.5 |
10.28 |
3050 |
1400 |
12800 |
5100 |
15 |
7 |
332 |
Stannum 5 |
|
|
|
|
9.94 |
|
|
11140 |
10060 |
18.1 |
15.3 |
350 |
|